1、5-47SSPC-PS 9.01November 1, 1982Editorial Revisions November 1, 2004SSPC: The Society for Protective CoatingsPAINTING SYSTEM NO. 9.01Cold-Applied Asphalt Mastic Painting System with Extra-Thick Film1. Scope1.1 This specifi cation covers a cold-applied asphalt mastic painting system for above-ground
2、steel structures.1.2 This system is suitable for use on parts or structures exposed in Environmental Zones 2A (frequently wet by fresh water), 2B (frequently wet by salt water), 3B (chemical, neutral), and 3C (chemical, alkaline). It should not be used in contact with oils, solvents, or other reagen
3、ts which tend to soften or attack the coating.2. Description2.1 This painting system consists of surface preparation by commercial blast cleaning or pickling and one thick or two thin coats of cold-applied asphalt mastic.3. Referenced Standards3.1 The latest issue, revision, or amendment of the refe
4、r-enced standards in effect on the date of invitation to bid shall govern, unless otherwise specifi ed.3.2 If there is a confl ict between the requirements of any of the cited referenced standards and this specifi cation, the requirements of this specifi cation shall prevail.3.3 SSPC STANDARDS AND J
5、OINT STANDARDS:PA 1 Shop, Field, and Maintenance Painting of SteelPA 2 Measurement of Dry Coating Thickness With Magnetic GagesPA Guide 4 Guide to Maintenance Re-painting with Oil Base or Alkyd Painting SystemsPaint 12 Cold Applied Asphalt Mastic (Extra Thick Film)SP 5/NACE No. 1 White Metal Blast C
6、leaningSP 6/NACE No. 3 Commercial Blast CleaningSP 8 PicklingSP 10/NACE No. 2 Near-White Blast Cleaning3.4 AMERICAN SOCIETY FOR TESTING AND MATERIALS (ASTM) STANDARD:D 3925 Standard Practice for Sampling Liquid Paints and Related Pigmented Coatings4. Surface Preparation4.1 SSPC-SP 6, “Commercial Bla
7、st Cleaning,” or SSPC-SP 8, “Pickling.” If specifi ed in the procurement documents better degrees of cleaning shall be substituted (SSPC-SP 5, “White Metal Blast Cleaning,” or SSPC-SP 10, “Near- White Blast Cleaning”).5. Paints5.1 COATING: SSPC-Paint 12, “Cold-Applied Asphalt Mastic (Extra Thick Fil
8、m).”6. Paint Application6.1 PAINT APPLICATION: Follow the requirements SSPC-PA 1, “Shop, Field, and Maintenance Painting of Steel.”6.2 TOUCH-UP PAINTING: In accordance with specifi ca-tion SSPC-PA 1, “Shop, Field, and Maintenance Painting of Steel,” and in particular with the section thereof entitle
9、d “Field Painting.”6.3 MAINTENANCE PAINTING: This specifi cation ap-plies to maintenance painting, provided specifi c instructions are included on the degree and amount of solvent cleaning, spot cleaning, spot priming, priming, and fi nish painting. For additional information on maintenance painting
10、 procedures, see SSPC-PA Guide 4, “Guide to Maintenance Repainting with Oil Base or Alkyd Painting Systems.”6.4 NUMBER OF COATS: Minimum of one.6.5 DRY FILM THICKNESS OF PAINT SYSTEM: Not less than the following as measured in accordance with SSPC- PA 2, “Measurement of Dry Coating Thickness with Ma
11、gnetic Gages”: 1600 micrometers (63 mils).7. Inspection7.1 All work and materials supplied under this specifi ca-tion are subject to timely inspection by the purchaser or his authorized representative. The contractor shall correct such work or replace such material as is found defective under this s
12、pecifi cation (See Note 9.1.). In case of dispute, unless otherwise specifi ed, the arbitration or settlement procedure established in the procurement documents shall be followed. If no arbitration or settlement procedure is established, then a procedure mutually agreeable to purchaser, material sup
13、plier, 5-48SSPC-PS 9.01November 1, 1982Editorial Revisions November 1, 2004and contractor shall be used. 7.2 Samples of paints under this painting system may be requested by the purchaser and shall be supplied upon request along with the manufacturers name and identifi cation for the materials. Samp
14、les may be requested at the time the purchase order is placed, or may be taken from unopened containers at the job site.7.3 Unless otherwise specifi ed, the sampling shall be in accordance with ASTM D 3925.8. Disclaimer8.1 While every precaution is taken to ensure that all information furnished in S
15、SPC standards and specifi cations is as accurate, complete, and useful as possible, SSPC cannot assume responsibility nor incur any obligation resulting from the use of any materials, coatings, or methods specifi ed herein, or of the specifi cation or standard itself.8.2 This specifi cation does not
16、 attempt to address problems concerning safety associated with its use. The user of this specifi cation, as well as the user of all products or practices described herein, is responsible for instituting appropriate health and safety practices and for insuring compliance with all governmental regulations.9. NoteNotes are not a requirement of this specifi cation. 9.1 The procurement documents should establish the responsibility for samples, testing, and any required affi davit certifying full compliance with the specifi cation.