1、| | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | | BRITISH STANDARD BS EN 10132-3:2000 Incorp
2、orating Corrigendum No.1 The European Standard EN 10132-3:2000 has the status of a British Standard ICS 77.140.10; 77.140.50 NO COPYING WITHOUT BSI PERMISSION EXCEPT AS PERMITTED BY COPYRIGHT LAW Cold rolled narrow steel strip for heat treatment Technical delivery conditions Part 3: Steels for quenc
3、hing and temperingThis British Standard, having been prepared under the direction of the Engineering Sector Committee, was published under the authority of the Standards Committee and comes into effect on 15 May 2000 BSI 07-2000 ISBN 0 580 35851 8 BS EN 10132-3:2000 Amendments issued since publicati
4、on Amd. No. Date Comments 11006 Corrigendum No.1 July 2000 Corrections to superscript and inferior characters in Table 3 National foreword This British Standard is the official English language version of EN 10132-3:2000. Together with BS EN 10132-1 and BS EN 10132-2, it supersedes BS 1449-1.15:1991
5、 which is withdrawn. The UK participation in its preparation was entrusted to Technical Committee ISE/31, Wrought steels, which has the responsibility to: aid enquirers to understand the text; present to the responsible European committee any enquiries on the interpretation, or proposals for change,
6、 and keep the UK interests informed; monitor related international and European developments and promulgate them in the UK. A list of organizations represented on this committee can be obtained on request to its secretary. Cross-references The British Standards which implement international or Europ
7、ean publications referred to in this document may be found in the BSI Standards Catalogue under the section entitled “International Standards Correspondence Index”, or by using the “Find” facility of the BSI Standards Electronic Catalogue. A British Standard does not purport to include all the neces
8、sary provisions of a contract. Users of British Standards are responsible for their correct application. Compliance with a British Standard does not of itself confer immunity from legal obligations. Summary of pages This document comprises a front cover, an inside front cover, the EN title page, pag
9、es 2 to 12, an inside back cover and a back cover. The BSI copyright notice displayed in this document indicates when the document was last issued.EUROPEAN STANDARD NORME EUROPENNE EUROPISCHE NORM EN 10132-3 February 2000 ICS 77.140.10; 77.140.50 English version Cold rolled narrow steel strip for he
10、at treatment - Technical delivery conditions - Part 3: Steels for quenching and tempering Feuillards lamins froid pour traitement thermique - Conditions techniques de livraison - Partie 3: Acier pour trempe et revenu Kaltband aus Stahl fr eine Wrmebehandlung - Technische Lieferbedingungen - Teil 3:
11、Vergtungssthle This European Standard was approved by CEN on 3 January 2000. CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this European Standard the status of a national standard without any alteration. Up-to-date lists and bibli
12、ographical references concerning such national standards may be obtained on application to the Central Secretariat or to any CEN member. This European Standard exists in three official versions (English, French, German). A version in any other language made by translation under the responsibility of
13、 a CEN member into its own language and notified to the Central Secretariat has the same status as the official versions. CEN members are the national standards bodies of Austria, Belgium, Czech Republic, Denmark, Finland, France, Germany, Greece, Iceland, Ireland, Italy, Luxembourg, Netherlands, No
14、rway, Portugal, Spain, Sweden, Switzerland and United Kingdom. EUROPEAN COMMITTEE FOR STANDARDIZATION COMIT EUROPEN DE NORMALISATION EUROPISCHES KOMITEE FR NORMUNG Central Secretariat: rue de Stassart, 36 B-1050 Brussels 2000 CEN All rights of exploitation in any form and by any means reserved world
15、wide for CEN national Members. Ref. No. EN 10132-3:2000 EPage 2 EN 10132-3:2000 BSI 07-2000 Contents Page Foreword 3 1 Scope 4 2 Normative references 4 3 Terms and definitions 4 4 Classification and designation 4 4.1 Classification 4 4.2 Designation 4 5 Information to be supplied by the purchaser 4
16、6 Manufacturing process 4 7 Requirements 5 7.1 General 5 7.2 Method of delivery 5 7.3 Delivery condition 5 7.4 Chemical composition 5 7.5 Mechanical properties 5 7.6 Structure 6 7.7 Surface finish 6 7.8 Dimensions and tolerances on dimensions and shape 6 8 Inspection 6 9 Sampling 6 10 Test methods 6
17、 11 Labelling, packaging and protection 7 12 Retests 7 Annex A (informative): Technical information on steels for 10 quenching and tempering Annex B (informative): List of corresponding former national designations 12Page 3 EN 10132-3:2000 BSI 07-2000 Foreword This European Standard has been prepare
18、d by Technical Committee ECISS/TC 23, Steels for heat treatment, alloy steels and free-cutting steels - Qualities and dimensions, the secretariat of which is held by DIN. This European Standard shall be given the status of a national standard, either by publication of an identical text or by endorse
19、ment, at the latest by August 2000, and conflicting national standards shall be withdrawn at the latest by August 2000. According to the CEN/CENELEC Internal Regulations, the national standards organizations of the following countries are bound to implement this European Standard: Austria, Belgium,
20、Czech Republic, Denmark, Finland, France, Germany, Greece, Iceland, Ireland, Italy, Luxembourg, Netherlands, Norway, Portugal, Spain, Sweden, Switzerland and the United Kingdom. The European Standard EN 10132, Cold rolled narrow steel strip for heat-treatment - Technical delivery conditions, is subd
21、ivided as follows: Part 1: General; Part 2: Case hardening steels; Part 3: Steels for quenching and tempering; Part 4: Spring steels and other special applications.Page 4 EN 10132-3:2000 BSI 07-2000 1 Scope 1.1 This part of EN 10132 applies to non-alloy and alloy cold rolled narrow steel strip in th
22、icknesses up to 6 mm for quenching and tempering, and in the quenched and tempered condition with thicknesses between 0,30 mm and 3,00 mm for general and for specific applications. 1.2 This EN 10132-3 is complemented by EN 10132-1. 2 Normative references This European Standard incorporates by dated
23、or undated reference, provisions from other publications. These normative references are cited at the appropriate places in the text and the publications are listed hereafter. For dated references, subsequent amendments to or revisions of any of these publications apply to this European Standard onl
24、y when incorporated in it by amendment or revision. For undated references the latest edition of the publication referred to applies. EN 10020, Definition and classification of grades of steel. EN 10132-1, Cold rolled narrow steel strip for heat treatment - Technical delivery conditions - Part 1: Ge
25、neral. EN 10140, Cold rolled narrow steel strip - Tolerances on dimensions and shape. EN ISO 6508-1, Metallic materials - Rockwell hardness test - Part 1: Test method (scales A, B, C, D, E, F, G, H, K, N, T) (ISO 6508-1:1999). 3 Terms and definitions For the purposes of this standard, the terms and
26、definitions given in EN 10132-1 apply. 4 Classification and designation 4.1 Classification All steels covered by this European Standard are classified according to EN 10020. Steel grades C22E, C30E, C35E, C40E, C45E, C50E, C55E, C60E and 25Mn4 are non-alloy special steels, steel grades 25CrMo4, 34Cr
27、Mo4 and 42CrMo4 are alloy special steels. 4.2 Designation See EN 10132-1. 5 Information to be supplied by the purchaser See EN 10132-1.Page 5 EN 10132-3:2000 BSI 07-2000 6 Manufacturing process See EN 10132-1. 7 Requirements 7.1 General See EN 10132-1. 7.2 Method of delivery See EN 10132-1. 7.3 Deli
28、very condition Cold rolled narrow steel strip covered by EN 10132-3 shall be supplied in one of the following delivery conditions: annealed or annealed and skin passed (+A or +LC); cold rolled (+CR); quenched and tempered (+QT) - for the grades indicated in Table 3 of this standard. NOTE The deliver
29、y condition - annealed to achieve spheroidized carbides (+AC) - may be agreed. In such cases, limits on spheroidization and mechanical properties may also be agreed at the time of enquiry and order. 7.4 Chemical composition 7.4.1 Cast analysis The chemical composition shall be in accordance with the
30、 values specified in Table 1 for the cast analysis. 7.4.2 Product analysis In cases where a product analysis is requested, the admissible deviations from the values specified for the cast analysis are indicated in Table 2. 7.5 Mechanical properties The mechanical properties of the strip shall be in
31、accordance with the values given in Table 3. For thicknesses outside this range, mechanical properties shall be agreed between the customer and the supplier. NOTE 1 For those customers who specify Rockwell hardness rather than Vickers hardness or tensile strength, a table is given in A.1, showing Ro
32、ckwell hardness values for information. NOTE 2 For information, the minimum hardness values given in Table A.2 show the minimum values after quenching, without tempering.Page 6 EN 10132-3:2000 BSI 07-2000 7.6 Structure 7.6.1 Grain size See EN 10132-1. 7.6.2 Non-metallic inclusions See EN 10132-1. 7.
33、6.3 Decarburization For steels with minimum carbon contents 0,50 %, decarburization shall not exceed 3 % of the material thickness per side when measured at a distance of 5 mm from the strip edge (see also EN 10132-1). 7.7 Surface finish The surface finish of cold rolled steel strip shall be bright
34、as achieved by rolling and annealing in a controlled atmosphere. The surface finishes of quenched and tempered cold rolled strip are as follows: grey/blue oxide finish: unpolished; bright tempered: unpolished; polished: obtained by fine grinding, abrasive brushing or other processes; polished and co
35、loured: blue or yellow colour obtained by oxidization by heattreatment. 7.8 Dimensions and tolerances on dimensions and shape Tolerances on width for quenched and tempered strip shall be agreed between customer and supplier. For all other tolerances EN 10140 applies (see also EN 10132-1). Special ed
36、ges are available by agreement between supplier and customer, and the tolerances on width for these edges are to be agreed. 8 Inspection See EN 10132-1. 9 Sampling See EN 10132-1. 10 Test methods See EN 10132-1.Page 7 EN 10132-3:2000 BSI 07-2000 11 Labelling, packaging and protection See EN 10132-1.
37、 12 Retests See EN 10132-1.Page 8 EN 10132-3:2000 BSI 07-2000 Table 1 - Chemical composition of steels for quenching and tempering a (cast analysis) Steel designation % by mass name number C Si max. Mn P max. S max. Cr Mo Ni max. C22E 1.1151 0,17 to 0,24 0,40 0,40 to 0,70 0,035 0,035 max. 0,40 max.
38、0,10 0,40 C30E 1.1178 0,27 to 0,34 0,40 0,50 to 0,80 0,035 0,035 max. 0,40 max. 0,10 0,40 C35E 1.1181 0,32 to 0,39 0,40 0,50 to 0,80 0,035 0,035 max. 0,40 max. 0,10 0,40 C40E 1.1186 0,37 to 0,44 0,40 0,50 to 0,80 0,035 0,035 max. 0,40 max. 0,10 0,40 C45E 1.1191 0,42 to 0,50 0,40 0,50 to 0,80 0,035 0
39、,035 max. 0,40 max. 0,10 0,40 C50E 1.1206 0,47 to 0,55 0,40 0,60 to 0,90 0,035 0,035 max. 0,40 max. 0,10 0,40 C55E 1.1203 0,52 to 0,60 0,40 0,60 to 0,90 0,035 0,035 max. 0,40 max. 0,10 0,40 C60E 1.1221 0,57 to 0,65 0,40 0,60 to 0,90 0,035 0,035 max. 0,40 max. 0,10 0,40 25Mn4 1.1177 0,23 to 0,28 0,40
40、 0,95 to 1,15 0,035 0,035 max. 0,40 max. 0,10 0,40 25CrMo4 1.7218 0,22 to 0,29 0,40 0,60 to 0,90 0,035 0,035 0,90 to 1,20 0,15 to 0,30 - 34CrMo4 1.7220 0,30 to 0,37 0,40 0,60 to 0,90 0,035 0,035 0,90 to 1,20 0,15 to 0,30 - 42CrMo4 1.7225 0,38 to 0,45 0,40 0,60 to 0,90 0,035 0,035 0,90 to 1,20 0,15 t
41、o 0,30 - a Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser, other t han for the purpose of finishing the heat. All reasonable precautions shall be taken to prevent the addition, from scrap or other material used in manufacture, o
42、f such elements which affect the hardenability, mechanical properties and application. Table 2 - Permissible deviations between the product analysis and the limiting values given in Table 1 for the cast analysis Element Permissible maximum content in the cast analysis % by mass Permissible deviation
43、 a % by mass C 0,55 0,55 0,65 0,02 0,03 Si 0,40 +0,03 Mn 0,95 0,95 1,15 0,04 0,05 P 0,035 +0,005 S 0,035 +0,005 Cr 0,40 0,40 1,20 +0,03 0,04 Mo 0,10 0,10 0,30 +0,02 0,03 Ni 0,40 +0,04 a means that in one cast the devation may occur over the upper value or under the lower value of the specified range
44、 in Table 1, but not both at the same time.Page 9 EN 10132-3:2000 BSI 07-2000 Table 3 - Mechanical properties and hardness requirements a, b delivery condition Steel designation annealed (+A) or annealed and skin passed (+LC) cold rolled c(+CR) quenched and tempered d(+QT) name number R p0,2e e N/mm
45、 Max. R m e N/mm max. A 80 e % min. HV e max. R m e N/mm max. HV e max. R m e N/mm HV e C22E 1.1151 400 500 22 155 900 265 - - C30E 1.1178 420 520 20 165 920 270 - - C35E 1.1181 430 540 19 170 930 275 - - C40E 1.1186 440 550 18 170 970 280 - - C45E 1.1191 455 570 18 180 1 020 290 - - C50E 1.1206 465
46、 580 17 180 1 050 295 1 050 to 1650 325 to 505 C55E 1.1203 480 600 17 185 1 070 300 1 100 to 1700 340 to 520 C60E 1.1221 495 620 17 195 1 100 305 1 150 to 1750 345 to 530 25Mn4 1.1177 460 590 20 180 f f - - 25CrMo4 1.7218 440 580 19 175 f f 990 to 1400 305 to 435 34CrMo4 1.7220 460 600 16 185 f f 1
47、020 to 1500 315 to 465 42CrMo4 1.7225 480 620 15 195 f f 1 100 to 1600 340 to 490 a The customer may specify hardness or tensile values but not both. If neither is specified then tensile values shall apply. b Values apply to thicknesses 0,30 mm t 3,00 mm. For thicker strip, the values for the mechan
48、ical properties shall be agreed at the time of enquiry and order. c For material supplied in the cold rolled condition, a range of 150 N/mm or 50 HV shall apply, e.g. 700 N/mm to 850 N/mm or e.g. 200 HV to 250 HV. d For material supplied in the quenched and tempered condition, a range of 150 N/mm or
49、 50 HV shall apply, e.g. 1 150 N/mm to 1 300 N/mm or e.g. 350 HV to 400 HV. e R p0,2 0,2 %-Proof strength; R mTensile strength; A 80Elongation on a gauge length of 80 mm; HV Vickers hardness. f Cold rolled condition may be supplied on request. In this case, the mechanical properties shall be agreed at the time of enquiry and order.Page 10 EN 10132-3:2000 BSI 07-2000 Annex A (informative) Technical information on steels for quenching and tempering Table A.1 - Reference values for Rockwell hard