ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf

上传人:visitstep340 文档编号:536956 上传时间:2018-12-06 格式:PDF 页数:17 大小:332.08KB
下载 相关 举报
ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf_第1页
第1页 / 共17页
ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf_第2页
第2页 / 共17页
ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf_第3页
第3页 / 共17页
ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf_第4页
第4页 / 共17页
ASTM F606-2013 Standard Test Methods for Determining the Mechanical Properties of Externally and Internally Threaded Fasteners Washers Direct Tension Indicators and Rivets《测定外螺纹及内螺.pdf_第5页
第5页 / 共17页
亲,该文档总共17页,到这儿已超出免费预览范围,如果喜欢就下载吧!
资源描述

1、Designation: F606 13Standard Test Methods forDetermining the Mechanical Properties of Externally andInternally Threaded Fasteners, Washers, Direct TensionIndicators, and Rivets1This standard is issued under the fixed designation F606; the number immediately following the designation indicates the ye

2、ar of originaladoption or, in the case of revision, the year of last revision.Anumber in parentheses indicates the year of last reapproval.Asuperscriptepsilon () indicates an editorial change since the last revision or reapproval.This standard has been approved for use by agencies of the U.S. Depart

3、ment of Defense.1. Scope*1.1 These test methods cover establishment of proceduresfor conducting tests to determine the mechanical properties ofexternally and internally threaded fasteners, washers, directtension indicators, and rivets.1.2 Property requirements and the applicable tests for theirdeter

4、mination are specified in individual product standards. Inthose instances where the testing requirements are unique or atvariance with these standard procedures, the product standardshall specify the controlling testing requirements.1.3 These test methods describe mechanical tests for deter-mining t

5、he following properties:SectionFor Externally Threaded Fasteners: 3Product Hardness 3.1Proof Load 3.2.1Method 1, Length Measurement 3.2.3Method 2, Yield Strength 3.2.4Method 3, Uniform Hardness 3.2.5Axial Tension Testing of Full-Size Product 3.4Wedge Tension Testing of Full-Size Product 3.5Tension T

6、esting of Machined Test Specimens 3.6Total Extension at Fracture TestSingle Sheer Test3.73.8For Internally Threaded Fasteners: 4Product Hardness 4.1Proof Load Test 4.2Cone Proof Load Test 4.3For Washers and Direct Tension Indicators: 5Product Hardness-General Requirements 5.1Through Hardened Washers

7、 5.2Carburized Washers 5.3Stainless Steel and Nonferrous Washers 5.4Direct Tension Indicators 5.5Compression Load 5.6For Rivets: 6Product Hardness 6.1Test for Embrittlement of Metallic-Coated Externally ThreadedFasteners7Test Method for Determining Decarburization and Carburization 81.4 The values s

8、tated in inch-pound units are to be regardedas standard. No other units of measurement are included in thisstandard.NOTE 1Acomplete metric companion to Test Methods F606 has beendevelopedF606M; therefore, no metric equivalents are shown in thesetest methods.1.5 This standard does not purport to addr

9、ess all of thesafety concerns, if any, associated with its use. It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use.2. Referenced Documents2.1 ASTM Standards:2A394 Specifica

10、tion for Steel Transmission Tower Bolts,Zinc-Coated and BareE4 Practices for Force Verification of Testing MachinesE8/E8M Test Methods for Tension Testing of Metallic Ma-terialsE10 Test Method for Brinell Hardness of Metallic MaterialsE18 Test Methods for Rockwell Hardness of Metallic Ma-terialsE83

11、Practice for Verification and Classification of Exten-someter SystemsE92 Test Method for Vickers Hardness of Metallic Materials(Withdrawn 2010)3E384 Test Method for Knoop and Vickers Hardness ofMaterialsF436 Specification for Hardened Steel WashersF606M Test Methods for Determining the Mechanical Pr

12、op-erties of Externally and Internally Threaded Fasteners,Washers, and Rivets (Metric)1These test methods are under the jurisdiction of ASTM Committee F16 onFasteners and are the direct responsibility of Subcommittee F16.01 on TestMethods.Current edition approved Nov. 1, 2013. Published December 201

13、3. Originallyapproved in 1979. Last previous edition approved in 2011 as F606 11a. DOI:10.1520/F0606-13.2For referenced ASTM standards, visit the ASTM website, www.astm.org, orcontact ASTM Customer Service at serviceastm.org. For Annual Book of ASTMStandards volume information, refer to the standard

14、s Document Summary page onthe ASTM website.3The last approved version of this historical standard is referenced onwww.astm.org.*A Summary of Changes section appears at the end of this standardCopyright ASTM International, 100 Barr Harbor Drive, PO Box C700, West Conshohocken, PA 19428-2959. United S

15、tates1F959 Specification for Compressible-Washer-Type DirectTension Indicators for Use with Structural FastenersF1624 Test Method for Measurement of Hydrogen Em-brittlement Threshold in Steel by the Incremental StepLoading TechniqueF2328 Test Method for Determining Decarburization andCarburization i

16、n Hardened and Tempered Threaded SteelBolts, Screws and Studs2.2 Military Standard:4MIL STD 1312, Test 13 and Test 203. Test Methods for Externally Threaded Fasteners3.1 Product HardnessTests shall be conducted after theremoval of any surface oxide, decarburization, plating or othercoating. All read

17、ings shall be within the hardness values listedin the product specification. The average of all readings on thesame part shall be considered as the product hardness. Testresults shall conform to the product specification for the lotrepresented by the test specimens to be considered conforming.Test s

18、pecimen preparation and hardness tests shall be con-ducted in accordance with Test Methods E18 for Rockwelltests, Test Method E10 for Brinell tests, Test Method E92 forVickers tests, or Test Method E384 for Microhardness tests.The method used is at the option of the manufacturer, withregards to the

19、size and grade of the products.3.1.1 Routine Test LocationsFor testing the hardness ofthe finished product, the following test locations can be used:3.1.1.1 For hex and square head bolts; test shall be con-ducted on the wrench flats, top of head, unthreaded shank, endof bolt or at the arbitration lo

20、cation.3.1.1.2 For studs, products without parallel wrench flats andfor head styles other than hex and square; tests shall beconducted on the unthreaded shank, end of the bolt or stud orat the arbitration location.3.1.1.3 Stress relieved products (3.1.1.1 and 3.1.1.2) aremeasured anywhere on the sur

21、face or through the cross section.Refer to the product specification for particular test location oruse the arbitration location.3.1.1.4 The Rockwell Hardness Scale may be used for allproduct diameters; however, the Brinell hardness is limited toproducts over 112-in. nominal diameter.3.1.2 Laborator

22、y InspectionAfter observing 3.1 and 3.1.1,a minimum of three readings shall be taken on each sample offinished product.3.1.3 Arbitration Test LocationFor purposes of arbitrationbetween the purchaser and seller over reported test results,hardness tests shall be conducted at the mid-radius (r/2) of at

23、ransverse section through the threads taken at a distance ofapproximately one diameter from the point end of the bolt orone end of the stud. Four readings shall be taken from the pointend of the bolt or one end of the stud. Four readings shall betaken approximately 90 to one another on the same plan

24、e, ifproduct size permits. Smaller diameter products may also usethe opposite parallel surface area of the bolt head end assectioned above (see Fig. 1). The use of Brinell hardness islimited to product sizes greater than 214-in. nominal diameter.3.2 Tension TestsIt is preferred that bolts and studs

25、betested full size, and it is customary, when so testing, to specifya minimum ultimate load (or stress) in pounds-force (orpounds-force per square inch.) Sections 3.2 3.5 apply whentesting externally threaded fasteners full size. Section 3.6 shallapply where the individual product specifications per

26、mit theuse of machined specimens (see Test Methods E8/E8M).3.2.1 Proof LoadThe proof-load test consists of stressingthe product with a specified load that the product mustwithstand without measurable permanent set. Alternative testsfor determining the ability of a fastener to pass the proof-loadtest

27、 are the yield strength test and the uniform hardness test.Either Method 1 (3.2.3), Method 2 (3.2.4), or Method 3 (3.2.5)may be used, but Method 1 shall be the arbitration method incase of any dispute as to acceptance of the product (see TestMethods E8/E8M).4Available from Standardization Documents

28、Order Desk, DODSSP, Bldg. 4,Section D, 700 Robbins Ave., Philadelphia, PA 19111-5098, http:/www.dodssp.daps.mil.FIG. 1 Hardness Arbitration Test LocationF606 1323.2.2 In both Methods 1 and 2, assemble the product in thefixture of the tension testing machine so that six completethreads (except for he

29、avy hex structural bolts, which shall bebased on four threads) are exposed between the grips. This isobtained by freely running the nut or fixture to the threadrunout of the specimen and then unscrewing the specimen sixfull turns. For continuous thread bolts, at least six full threadsshall be expose

30、d between the fixture ends; however, for refereepurposes, six full threads shall be exposed.3.2.3 Method 1, Length MeasurementTo ensure consistentand repetitive length measurements of the fastener, thethreaded end and top of the bolt head shall have conicaldepressions made at the approximate axis or

31、 center line of thefastener. In the event of a dispute over test results the test shallbe conducted after the removal of all manufacturer or grademarkings, surface oxide, decarburization, plating, othercoating, or a combination thereof, to achieve a clean, flatsurface and the conical depressions sha

32、ll be created using alathe or some type of centering fixture. All debris shall beremoved from the conical depressions before measuring thepart. When fasteners are too long to test in the availableequipment they may be cut to 8 inches 6 0.125 and testedusing Method 1. If there is a dispute over resul

33、ts when testingthe same part or lot of parts both full size and cut to 8 inchesthe 8 inch test results shall be used to determine acceptance.The measuring instrument shall have pointed anvils whichmate with the center line depressions and be capable ofmeasuring changes in length of 0.0001 in. with a

34、n accuracy of0.0001 in. in any 0.001 in. range. Place the fastener betweenthe measuring anvils. The fastener shall be rotated at least 360degrees to assure sound seating. At the position where thelowest value is indicated the instrument shall be zeroed or theindicated measurement shall be recorded.

35、If using a boltextensometer, the bolt with attached extensometer may beassembled into the tension testing machine. If not, mark thefastener so it may be placed as close as possible to the sameposition for the second reading. Remove and assemble thefastener into the tension testing machine as outline

36、d in 3.4.With a test speed which shall not exceed 0.12 in./min, asdetermined with a free-running cross head, axially load thefastener to the proof load value specified in the productspecification. This load shall be maintained for a period of 10s before releasing the load. Replace the fastener betwe

37、en themeasuring anvils and rotate at least 360 degrees as before. Thefastener shall be stopped at the position where the lowest valueis indicated. The measurement shall show no permanentelongation. A tolerance of 60.0005 in. shall be allowed (formeasurement error only) between the measurement madebe

38、fore loading and that made after loading. Variables such asstraightness, thread alignment, or measurement error couldresult in apparent elongation of the product when the specifiedproof load is initially applied. In such cases, the product maybe retested using a 3 % greater load, and shall be consid

39、eredacceptable if there is no difference in the length measurementafter this loading within a 0.0005 in. measurement tolerance asoutlined.3.2.4 Method 2, Yield StrengthAssemble the product inthe testing equipment as outlined in 3.4.As the load is applied,measure and record the total elongation of th

40、e product or anypart of it that includes the exposed threads to produce aload-elongation diagram. Determine the load or stress at anoffset equal to 0.2 % of the length of bolt occupied by six fullthreads as shown in Fig. 2 (except for heavy hex structuralbolts, which shall be based on four threads)

41、by the methoddescribed in 3.6.3.1.3.2.4.1 Method 2A, Yield Strength for Austenitic StainlessSteel and Non-ferrous MaterialsAssemble the product in thetesting equipment as outlined in 3.4. As the load is applied,measure and record the total elongation of the product in orderto produce a load elongati

42、on diagram. Determine the load orstress at an offset equal to 0.2 % strain based on the length ofthe bolt between the holders as shown in Fig. 2, which will besubject to elongation under load by using the method describedin 3.6.3.1.FIG. 2 Tension Testing of Full-Size Bolt (Typical Set-Up)F606 1333.2

43、.5 Method 3, Uniform HardnessThe fasteners shall betested for hardness as described in 3.1, and in addition, thehardness shall also be determined in the core. The differencebetween the mid-radius and core hardness shall be not morethan 3 points on a Rockwell C Scale; and both readings mustbe within

44、product specification. This test is valid for fastenersup to and including 1 in. in diameter.3.3 Bolts or Studs Too Short for Tension TestingProductlengths less than those shown in Table 1 for product14 through34 in. in diameter and less than three diameters in length forproduct above34 in. in diame

45、ter, or that do not have sufficientthreads for proper engagement and still leave the specifiednumber of complete threads exposed between the grips, shallbe deemed too short for tension testing, and acceptance shall bebased on a hardness test performed in accordance with 3.1.Iftests other than produc

46、t hardness are required, their require-ments should be referenced in the product specification. Whendifferences in tensile testing lengths exist between this standardand product standards, the requirements of the product stan-dard shall take precedence. Minimum length in Table 1indicates the nominal

47、 specified length of the product (that is anA449 Hex Cap Screw size is specified as12-13118 indicates118 in. is the nominal length).3.4 Axial Tension Testing of Full-Size Products:3.4.1 Test bolts in a holder with the load axially appliedbetween the head and a nut or suitable fixture (Fig. 2), eithe

48、r ofwhich shall have sufficient thread engagement to develop thefull strength of the product. Assemble the nut or fixture on theproduct, leaving a minimum of six complete bolt threadsexposed between the grips except for heavy hex structuralbolts, which shall have four complete threads exposed betwee

49、nthe grips.3.4.2 Test studs by assembling one end in the threadedfixture to the thread runout. For studs having unlike threads,this shall be the end with the finer pitch thread, or with thelarger minor diameter. Likewise, assemble the other end of thestud in a threaded fixture, leaving six complete threads exposedbetween the grips. For continuous thread studs, at least sixcomplete threads shall be exposed between the fixture ends.The maximum speed of the free-running cross head shall notexceed 1 in./min. When reporting the tensile strength ofproduct, in p

展开阅读全文
相关资源
猜你喜欢
  • ASTM C882 C882M-2013 Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf ASTM C882 C882M-2013 Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf
  • ASTM C882 C882M-2013a Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf ASTM C882 C882M-2013a Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf
  • ASTM C882-2005 Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf ASTM C882-2005 Standard Test Method for Bond Strength of Epoxy-Resin Systems Used With Concrete By Slant Shear《斜切法测定混凝土用环氧树脂粘结剂的粘结强度的标准试验方法》.pdf
  • ASTM C884 C884M-1998(2005) Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf ASTM C884 C884M-1998(2005) Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf
  • ASTM C884 C884M-1998(2010) Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf ASTM C884 C884M-1998(2010) Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf
  • ASTM C884 C884M-2016 Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf ASTM C884 C884M-2016 Standard Test Method for Thermal Compatibility Between Concrete and an Epoxy-Resin Overlay《混凝土和环氧树脂涂层间热容性的标准试验方法》.pdf
  • ASTM C885-1987(2007) Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材的弹性模量的标准试验方法》.pdf ASTM C885-1987(2007) Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材的弹性模量的标准试验方法》.pdf
  • ASTM C885-1987(2007)e1 Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材的弹性模量的标准试验方法》.pdf ASTM C885-1987(2007)e1 Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材的弹性模量的标准试验方法》.pdf
  • ASTM C885-1987(2012) Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材弹性模量的标准试验方法》.pdf ASTM C885-1987(2012) Standard Test Method for Youngs Modulus of Refractory Shapes by Sonic Resonance《用音响共振法测定耐火异型材弹性模量的标准试验方法》.pdf
  • 相关搜索

    当前位置:首页 > 标准规范 > 国际标准 > ASTM

    copyright@ 2008-2019 麦多课文库(www.mydoc123.com)网站版权所有
    备案/许可证编号:苏ICP备17064731号-1