1、BRITISH STANDARDBS EN10083-2:2006Steels for quenching and tempering Part 2: Technical delivery conditions for non alloy steelsThe European Standard EN 10083-2:2006 has the status of a British StandardICS 77.140.10g49g50g3g38g50g51g60g44g49g42g3g58g44g55g43g50g56g55g3g37g54g44g3g51g40g53g48g44g54g54g
2、44g50g49g3g40g59g38g40g51g55g3g36g54g3g51g40g53g48g44g55g55g40g39g3g37g60g3g38g50g51g60g53g44g42g43g55g3g47g36g58BS EN 10083-2:2006This British Standard was published under the authority of the Standards Policy and Strategy Committee on 31 August 2006 BSI 2006ISBN 0 580 49098 XNational forewordThis
3、British Standard is the official English language version of EN 10083-2:2006. It supersedes BS EN 10083-2:1991 which is withdrawn.The UK participation in its preparation was entrusted to Technical Committee ISE/31, Wrought steels, which has the responsibility to: A list of organizations represented
4、on this committee can be obtained on request to its secretary.Cross-referencesThe British Standards which implement international or European publications referred to in this document may be found in the BSI Catalogue under the section entitled “International Standards Correspondence Index”, or by u
5、sing the “Search” facility of the BSI Electronic Catalogue or of British Standards Online.This publication does not purport to include all the necessary provisions of a contract. Users are responsible for its correct application. Compliance with a British Standard does not of itself confer immunity
6、from legal obligations. aid enquirers to understand the text; present to the responsible international/European committee any enquiries on the interpretation, or proposals for change, and keep UK interests informed; monitor related international and European developments and promulgate them in the U
7、K.Summary of pagesThis document comprises a front cover, an inside front cover, the EN title page, pages 2 to 37 and a back cover.The BSI copyright notice displayed in this document indicates when the document was last issued.Amendments issued since publicationAmd. No. Date CommentsEUROPEAN STANDARD
8、NORME EUROPENNEEUROPISCHE NORMEN 10083-2August 2006ICS 77.140.10 Supersedes EN 10083-2:1991 English VersionSteels for quenching and tempering - Part 2: Technical deliveryconditions for non alloy steelsAciers pour trempe et revenu - Partie 2: Conditionstechniques de livraison des aciers non allisVerg
9、tungssthle - Teil 2: Technische Lieferbedingungenfr unlegierte SthleThis European Standard was approved by CEN on 30 June 2006.CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this EuropeanStandard the status of a national standard w
10、ithout any alteration. Up-to-date lists and bibliographical references concerning such nationalstandards may be obtained on application to the Central Secretariat or to any CEN member.This European Standard exists in three official versions (English, French, German). A version in any other language
11、made by translationunder the responsibility of a CEN member into its own language and notified to the Central Secretariat has the same status as the officialversions.CEN members are the national standards bodies of Austria, Belgium, Cyprus, Czech Republic, Denmark, Estonia, Finland, France,Germany,
12、Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania,Slovakia, Slovenia, Spain, Sweden, Switzerland and United Kingdom.EUROPEAN COMMITTEE FOR STANDARDIZATIONCOMIT EUROPEN DE NORMALISATIONEUROPISCHES KOMITEE FR NORMUNGManagemen
13、t Centre: rue de Stassart, 36 B-1050 Brussels 2006 CEN All rights of exploitation in any form and by any means reservedworldwide for CEN national Members.Ref. No. EN 10083-2:2006: EEN 10083-2:2006 (E) 2 Contents Page Foreword3 1 Scope 4 2 Normative references 4 3 Terms and definitions .5 4 Classific
14、ation and designation.5 4.1 Classification5 4.2 Designation 5 5 Information to be supplied by the purchaser .6 5.1 Mandatory information6 5.2 Options .6 6 Manufacturing process .7 6.1 General7 6.2 Deoxidation 7 6.3 Heat treatment and surface condition at delivery 7 6.4 Cast separation7 7 Requirement
15、s.7 7.1 Chemical composition, hardenability and mechanical properties .7 7.2 Machinability 8 7.3 Shearability of semi-finished products and bars .8 7.4 Structure .8 7.5 Internal soundness9 7.6 Surface quality .9 7.7 Dimensions, tolerances on dimensions and shape.9 8 Inspection .10 8.1 Testing proced
16、ures and types of documents.10 8.2 Frequency of testing .10 8.3 Tests to be carried out for specific inspection.10 9 Preparation of samples and test pieces10 9.1 Selection and preparation of samples for chemical analysis .10 9.2 Location and orientation of samples and test pieces for mechanical test
17、s10 9.3 Location and preparation of samples for hardness and hardenability tests 11 9.4 Identification of samples and test pieces .11 10 Test methods11 10.1 Chemical analysis11 10.2 Mechanical tests 11 10.3 Hardness and hardenability tests 11 10.4 Retests 11 11 Marking, labelling, packaging.11 Annex
18、 A (normative) Options 34 Annex B (informative) Comparison of steel grades specified in this European Standard and ISO 683-1:1987 and other steel grades previously standardized nationally.36 Bibliography 37 EN 10083-2:2006 (E) 3 Foreword This document (EN 10083-2:2006) has been prepared by Technical
19、 Committee ECISS/TC 23 “Steels for heat treatment, alloy steels and free-cutting steels - Qualities and dimensions”, the secretariat of which is held by DIN. This European Standard shall be given the status of a national standard, either by publication of an identical text or by endorsement, at the
20、latest by February 2007, and conflicting national standards shall be withdrawn at the latest by February 2007. This document supersedes EN 10083-2:1991. Together with Part 1 and Part 3 of this standard, this Part 2 is a revision of the following European Standards: EN 10083-1:1991 +A1:1996, Quenched
21、 and tempered steels Part 1: Technical delivery conditions for special steels EN 10083-2: 1991 +A1:1996, Quenched and tempered steels Part 2: Technical delivery conditions for unalloyed quality steels EN 10083-3:1995, Quenched and tempered steels Part 3: Technical delivery conditions for boron steel
22、s and of EURONORM 86-70, Flame and induction hardening steels Quality specifications According to the CEN/CENELEC Internal Regulations, the national standards organizations of the following countries are bound to implement this European Standard: Austria, Belgium, Cyprus, Czech Republic, Denmark, Es
23、tonia, Finland, France, Germany, Greece, Hungary, Iceland, Ireland, Italy, Latvia, Lithuania, Luxembourg, Malta, Netherlands, Norway, Poland, Portugal, Romania, Slovakia, Slovenia, Spain, Sweden, Switzerland and United Kingdom. EN 10083-2:2006 (E) 4 1 Scope This part of EN 10083, in addition to Part
24、 1, specifies the technical delivery requirements for: semi-finished products, hot formed, e.g. blooms, billets, slabs (see NOTES 2 and 3 in EN 10083-1:2006, Clause 1), bars (see NOTE 2 in EN 10083-1:2006, Clause 1), rod, wide flats, hot-rolled strip and sheet/plate, forgings (see NOTE 2 in EN 10083
25、-1:2006, Clause 1), manufactured from the direct hardening non alloy steels for quenching and tempering and the non alloy flame and induction hardening steels and supplied in one of the heat treatment conditions given for the different types of products in Table 1, lines 2 to 7, and in one of the su
26、rface conditions given in Table 2. The steels are generally intended for the manufacture of quenched and tempered, flame or induction hardened machine parts, but can also be used in the normalized condition. The requirements for mechanical properties given in this document are restricted to the size
27、s given in Table 9 and Table 10. NOTE This document does not apply for bright steel products. For bright steel products EN 10277-1 and EN 10277-5 apply. In special cases, variations in these technical delivery requirements or additions to them may be agreed at the time of enquiry and order (see Anne
28、x A). 2 Normative references The following referenced documents are indispensable for the application of this document. For dated references, only the edition cited applies. For undated references, the latest edition of the referenced document (including any amendments) applies. EN 10002-1, Metallic
29、 materials Tensile testing Part 1: Method of test at ambient temperature EN 10020, Definition and classification of grades of steel EN 10027-1, Designation systems for steels Part 1: Steel names EN 10027-2, Designation systems for steel Part 2: Numerical system EN 10045-1, Metallic materials Charpy
30、impact test Part 1: Test method EN 10083-1:2006, Steels for quenching and tempering Part 1: General technical delivery conditions EN 10160, Ultrasonic testing of steel flat product of thickness equal or greater than 6 mm (reflection method) EN 10163-2, Delivery requirements for surface condition of
31、hot-rolled steel plates, wide flats and sections Part 2: Plate and wide flats EN 10083-2:2006 (E) 5 EN 10204, Metallic products Types of inspection documents EN 10221, Surface quality classes for hot-rolled bars and rods Technical delivery conditions CR 10261, ECISS Information Circular 11 Iron and
32、steel Review of available methods of chemical analysis EN 10308, Non destructive testing Ultrasonic testing of steel bars EN ISO 377, Steel and steel products Location and preparation of samples and test pieces for mechanical testing (ISO 377:1997) EN ISO 642, Steel Hardenability test by end quenchi
33、ng (Jominy test) (ISO 642:1999) EN ISO 643, Steels Micrographic determination of the apparent grain size (ISO 643:2003) EN ISO 3887, Steels Determination of depth of decarburization (ISO 3887:2003) EN ISO 6506-1, Metallic materials Brinell hardness test Part 1: Test method (ISO 6506-1:2005) EN ISO 6
34、508-1:2005, Metallic materials Rockwell hardness test Part 1: Test method (scales A, B, C, D, E, F, G, H, K, N, T) (ISO 6508-1:2005) EN ISO 14284, Steel and iron Sampling and preparation of samples for the determination of chemical composition (ISO 14284:1996) EN ISO 18265, Metallic materials Conver
35、sion of hardness values (ISO 18265:2003) 3 Terms and definitions For the purposes of this document, the terms and definitions given in EN 10083-1:2006 apply. 4 Classification and designation 4.1 Classification Steel grades C35, C40, C45, C55 and C60 are classified according to EN 10020 as non alloy
36、quality steels and the other steel grades as non alloy special steels. 4.2 Designation 4.2.1 Steel names For the steel grades covered by this document, the steel names as given in the relevant tables are allocated in accordance with EN 10027-1. 4.2.2 Steel numbers For the steel grades covered by thi
37、s document, the steel numbers as given in the relevant tables are allocated in accordance with EN 10027-2. EN 10083-2:2006 (E) 6 5 Information to be supplied by the purchaser 5.1 Mandatory information See EN 10083-1:2006, 5.1. 5.2 Options A number of options are specified in this document (listed be
38、low). If the purchaser does not indicate his wish to implement any of these options, the supplier shall act in accordance with the basic specification. a) any particular heat treatment condition (see 6.3.2); b) any particular surface condition (see 6.3.3); c) any verification of the product analysis
39、 (see 7.1.2.2 and A.6); d) any requirement to the hardenability (+H, +HH, +HL) for special steels (see 7.1.3) and if agreed the information concerning calculating hardenability (see 10.3.2); e) any verification of mechanical properties of reference test pieces in the quenched and tempered (+QT) or n
40、ormalized (+N) condition (see A.1 and A.2); f) any fine grain requirements (see 7.4 and A.3); g) any requirements for the verification of non-metallic inclusion content of special steels (see 7.4 and A.4); h) any requirement for internal soundness (see 7.5 and A.5); i) any requirement relating to su
41、rface quality (see 7.6.3); j) any requirement regarding the permissible depth of decarburization of special steels (see 7.6.4); k) suitability of bars and rod for bright drawing (see 7.6.5); l) any requirement relating to removal of surface defects (see 7.6.6); m) inspection of surface condition and
42、 dimensions shall be carried out by the purchaser at the manufacturers works (see 8.1.4); n) any requirement concerning special marking of the products (see Clause 11 and A.7). EXAMPLE 20 round bars with the nominal diameter 20 mm and the nominal length of 8000 mm according to EN 10060 made of steel
43、 grade C45E (1.1191), according to EN 10083-2 in the heat treatment condition +A, inspection certificate 3.1 as specified in EN 10204. 20 round bars EN 10060 - 20x8000 EN 10083-2 C45E+A EN 10204 - 3.1 or 20 round bars EN 10060 - 20x8000 EN 10083-2 1.1191+A EN 10204 - 3.1 EN 10083-2:2006 (E) 7 6 Manu
44、facturing process 6.1 General The manufacturing process of the steel and of the products is left to the discretion of the manufacturer with the restrictions given by the requirements in 6.2 to 6.4. 6.2 Deoxidation All steels shall be killed. 6.3 Heat treatment and surface condition at delivery 6.3.1
45、 Untreated condition Unless otherwise agreed at the time of enquiry and order, the products shall be delivered in the untreated, i.e. hot worked, condition. NOTE Depending on product shape and dimensions, not all steel grades can be delivered in the hot worked untreated condition (e. g. steel grade
46、C60). 6.3.2 Particular heat treatment condition If so agreed at the time of enquiry and order, the products shall be delivered in one of the heat-treatment conditions given in Table 1, lines 3 to 7. 6.3.3 Particular surface condition If so agreed at the time of enquiry and order, the products shall
47、be delivered with one of the particular surface conditions given in Table 2, lines 3 to 7. 6.4 Cast separation The products shall be delivered separated by cast. 7 Requirements 7.1 Chemical composition, hardenability and mechanical properties 7.1.1 General Table 1 shows the combinations of usual hea
48、t-treatment conditions at delivery, product forms and requirements as specified in Tables 3 to 10. Except where special steels are ordered in the quenched and tempered condition, the special steels may be supplied with or without hardenability requirements (see Table 1, columns 8 and 9). 7.1.2 Chemi
49、cal composition 7.1.2.1 The chemical composition determined by cast analysis shall comply with the values in Table 3. 7.1.2.2 Permissible deviations between the limiting values for cast analysis and the values for product analysis are given in Table 4. The product analysis shall be carried out when specified at the time of the enquiry and order (see A.6). EN 10083-2:2006 (E) 8 7.1.3 Hardenability Where the steel is ordered by using the symbols for normal (+H) or restricted (+HL, +HH) hardenability requ