FORD WSE-M2D401-A3-2004 FLUOROELASTOMER (FKM) OXYGENATED OXIDIZED FUEL RESISTANT COMPRESSION STRESS RELAXATION RESISTANT LOW TEMPERATURE RESISTANT O-RING TO BE USED WITH FORD WSS-.pdf

上传人:eastlab115 文档编号:750079 上传时间:2019-01-14 格式:PDF 页数:4 大小:100.88KB
下载 相关 举报
FORD WSE-M2D401-A3-2004 FLUOROELASTOMER (FKM) OXYGENATED OXIDIZED FUEL RESISTANT COMPRESSION STRESS RELAXATION RESISTANT LOW TEMPERATURE RESISTANT O-RING  TO BE USED WITH FORD WSS-.pdf_第1页
第1页 / 共4页
FORD WSE-M2D401-A3-2004 FLUOROELASTOMER (FKM) OXYGENATED OXIDIZED FUEL RESISTANT COMPRESSION STRESS RELAXATION RESISTANT LOW TEMPERATURE RESISTANT O-RING  TO BE USED WITH FORD WSS-.pdf_第2页
第2页 / 共4页
FORD WSE-M2D401-A3-2004 FLUOROELASTOMER (FKM) OXYGENATED OXIDIZED FUEL RESISTANT COMPRESSION STRESS RELAXATION RESISTANT LOW TEMPERATURE RESISTANT O-RING  TO BE USED WITH FORD WSS-.pdf_第3页
第3页 / 共4页
FORD WSE-M2D401-A3-2004 FLUOROELASTOMER (FKM) OXYGENATED OXIDIZED FUEL RESISTANT COMPRESSION STRESS RELAXATION RESISTANT LOW TEMPERATURE RESISTANT O-RING  TO BE USED WITH FORD WSS-.pdf_第4页
第4页 / 共4页
亲,该文档总共4页,全部预览完了,如果喜欢就下载吧!
资源描述

1、 ENGINEERING MATERIAL SPECIFICATIONDate Action Revisions 2004 09 17 Revised Para 3.0 inserted; para 3.1, 3.2, 3.3, 3.15 Updated E. Duda1990 02 06 Released WSD-M4D401-A C10058098 B. HennesseyPrinted copies are uncontrolled Copyright 2004, Ford Global Technologies, LLC Page 1 of 4 FLUOROELASTOMER (FKM

2、), OXYGENATED/OXIDIZED WSD-M2D401-A FUEL RESISTANT, COMPRESSION STRESS RELAXATION RESISTANT, O-RING FLUOROELASTOMER (FKM), OXIDIZED FUEL WSE-M2D401-A2 RESISTANT, COMPRESSION STRESS RELAXATION RESISTANT, LOW TEMPERATURE RESISTANT, O-RING FLUOROELASTOMER (FKM), OXYGENATED/OXIDIZED WSE-M2D401-A3 FUEL R

3、ESISTANT, COMPRESSION STRESS RELAXATION RESISTANT, LOW TEMPERATURE RESISTANT, O-RING 1. SCOPE The material described by these specifications is a fluoroelastomer (FKM) O-ring with good resistance to highly aromatic fuels, including those containing methanol and ethanol (flex fuels). 2. APPLICATION T

4、hese specifications were released originally for material used in O-rings for use within the fuel system such as for sealing fuel injectors into the fuel rail. These materials have excellent resistance to stress relaxation, sour gas and automotive fuels insuring long-term sealability. WSE-M2D401-A2

5、and WSE-M2D401-A3 have good low temperature resistance and will remain serviceable down to -40 C. Of the three materials only WSE-M2D401-A3 can be used if resistance to both low temperatures and flex fuels e.g. gasoline and methanol, are required. 3. REQUIREMENTS 3.0 STANDARD REQUIREMENTS FOR PRODUC

6、TION MATERIALS Material suppliers and part producers must conform to the Companys Standard Requirements For Production Materials (WSS-M99P1111-A). 3.4 MATERIAL TESTING 3.4.1 Preparation of Test Specimens All tests shall be carried out on finished parts. When not feasible, specimens cut from molded t

7、est sheets manufactured from the same material and with equivalent cure to molded parts are recommended. The test sheets shall have the following dimensions: 150 x 150 mm, min x 2.0 +/- 0.2 mm ENGINEERING MATERIAL SPECIFICATIONWSD-M2D401-A/A2/A3Printed copies are uncontrolled Copyright 2004, Ford Gl

8、obal Technologies, LLC Page 2 of 4 3.5 ORIGINAL PROPERTIES A A2 A3 3.5.1 Hardness, International 67 - 80 68 - 82 60 - 74 (ISO 48/ASTM D 1415, micro method) 3.5.2 Tensile Strength, MPa, min 9.0 7.0 6.7 (ASTM D 1414, Section 8 or ISO 37/ASTM D 412 Die C) 3.5.3 Elongation at Break, 125 125 150 %, min (

9、ASTM D 1414, Section 8) 3.5.4 Compression Set, %, max 35 40 50 (ASTM D 1414, Section 10) 70 h at 200 +/- 2 C) 3.5.4.1 70 h at 130 C - 18% - 3.5.5 Tear Strength, kN/m, min 25 20.0 10.0 (ISO 34, Method B, Procedure (a)/ASTM D 624 Die C) 3.5.6 Ozone Resistance, Rating, max 0 0 0 (FLTM BP 101-01, Proced

10、ure A) 3.6 HEAT AGED (ISO 188/ASTM D 573, 150 +/- 50 air changes/h, 1,000 h at 200 +/- 2 C) 3.6.1 Hardness Change, max +10 +7 +7 3.6.2 Tensile Strength Change, -30 -30 -15 %, max 3.6.3 Elongation at Break -40 -12 to +20 -42 Change, %, max 3.7 HEAT AGED (ISO 188/ASTM D 573, 150 +/- 50 air changes/h,

11、168 h at 250 +/- 2 C) 3.7.1 Hardness Change, max +15 +10 +/- 10 (90 IRHD max value) 3.7.2 Tensile Strength Change, -15 -30 +30 to -60 %, max 3.7.3 Elongation at Break -40 -25 -20 to +50 Change, %, max (100% min value) ENGINEERING MATERIAL SPECIFICATIONWSD-M2D401-A/A2/A3Printed copies are uncontrolle

12、d Copyright 2004, Ford Global Technologies, LLC Page 3 of 4 3.8 IMMERSION IN ASTM FUEL C (ISO 1817/ASTM D 471, 168 h at 23 +/- 2 C) A A2 A3 3.8.1 Hardness Change, max -10 -14 -10/+5 3.8.2 Tensile Strength -35 -28 -30 Change, %, max 3.8.3 Elongation at Break -25 -30 -25 to +20 Change, %, max 3.8.4 Vo

13、lume Change, %, max +10 0/+10 0 to +12 3.9 IMMERSION IN 100% METHANOL (ISO 1817/ASTM D 471,168 h at 23 +/- 2 C) 3.9.1 Hardness Change, max - - -22 3.9.2 Tensile Strength Change, - - -55 %, max 3.9.3 Elongation Change, % - - -25 to +20 3.9.4 Volume Change, %, max - - +18 3.10 IMMERSION IN ASTM FUEL C

14、 +15% METHANOL (ISO 1817/ASTM D 471, 168 h at 23 +/- 2 C) 3.10.1 Hardness Change, max -25 -32 -22 3.10.2 Tensile Strength -70 -68 -55 Change, %, max 3.10.3 Elongation at Break -37 -30 -35 Change, %, max 3.10.4 Volume Change, % +5 to +37 0 to +48 0 to 22 3.11 IMMERSION IN ETHANOL FUELS The testing ca

15、rried out by immersion in methanol-containing fuels validates the material for use in ethanol-containing fuels. ENGINEERING MATERIAL SPECIFICATIONWSD-M2D401-A/A2/A3Printed copies are uncontrolled Copyright 2004, Ford Global Technologies, LLC Page 4 of 4 3.12 IMMERSION IN OXIDIZED (SOUR) FUEL (FLTM A

16、Z 105-01, PN 180, 336 h at 60 C) A A2 A3 3.12.1 Hardness Change, max -25 -45 -25 3.12.2 Tensile Strength Change, -70 -66 -60 %, max 3.12.3 Elongation at Break -37 -15 to +26 +30 Change, %, max 3.12.4 Volume Change, %, max +45 +45 0 to +28 3.13 COMPRESSION STRESS RELAXATION, 0.35 0.40 - F1000/Fo, min

17、 (ISO 6056 at 25% compression, carried out on finished parts) Measure the initial back-force (Fo) after 30 minutes at 23 +/- 2 C. Age at 150 +/- 2 C and take back-force (Ft) measurements at 23 +/- 2 C after 24, 48, 96, 168 h and thereafter every 168 h until a total elapsed test time of 1,000 h has b

18、een completed. Plot Ft/Fo against log 10 time in hours. 3.14 LOW TEMPERATURE FLEXIBILITY TEST, -18 -29 -21 TR10, C, max (ASTM D 1329) 5. GENERAL INFORMATION The information given below is provided for clarification and assistance in meeting the requirements of this specification. 5.1 IMMERSION IN 100% METHANOL (ISO 1817/ASTM D 471, 168 h at 23 +/- 2 C) 5.1.1 Hardness Change, max -30 -40 - 5.1.2 Tensile Strength Change, -60 -78 - %, max 5.1.3 Elongation at Break -20 -38 - Change, %, max 5.1.4 Volume Change, %, max +90 +120 -

展开阅读全文
相关资源
猜你喜欢
  • CEN TS 15717-2008 Parquet flooring - General guideline for installation《镶木地板 安装用通用指南》.pdf CEN TS 15717-2008 Parquet flooring - General guideline for installation《镶木地板 安装用通用指南》.pdf
  • CEN TS 15718-2011 Railway applications - Wheelsets and bogies - Product requirements for cast wheels《铁路应用 轮对和转向架 铸造车轮产品要求》.pdf CEN TS 15718-2011 Railway applications - Wheelsets and bogies - Product requirements for cast wheels《铁路应用 轮对和转向架 铸造车轮产品要求》.pdf
  • CEN TS 15731-2008 Cereals and cereal products - Common wheat (Triticum aestivum L ) - Determination of alveograph properties of dough at adapted hydration from commercial or test f.pdf CEN TS 15731-2008 Cereals and cereal products - Common wheat (Triticum aestivum L ) - Determination of alveograph properties of dough at adapted hydration from commercial or test f.pdf
  • CEN TS 15754-2008 Animal feeding stuffs - Determination of sugar content - High performance exchange chromatographic method (HPAEC-PAD)《牲畜饲料 含糖量的测定 高效交换色谱法(HPAEC-PAD)》.pdf CEN TS 15754-2008 Animal feeding stuffs - Determination of sugar content - High performance exchange chromatographic method (HPAEC-PAD)《牲畜饲料 含糖量的测定 高效交换色谱法(HPAEC-PAD)》.pdf
  • CEN TS 15790-2008 Animal feeding stuffs - PCR typing of probiotic strains of Saccharomyces cerevisiae (yeast)《牲畜饲料 聚合酶连锁反应测定酿酒酵母(酵母目)前生命期同类的PCR类型》.pdf CEN TS 15790-2008 Animal feeding stuffs - PCR typing of probiotic strains of Saccharomyces cerevisiae (yeast)《牲畜饲料 聚合酶连锁反应测定酿酒酵母(酵母目)前生命期同类的PCR类型》.pdf
  • CEN TS 15810-2008 Graphical symbols for use on integrated building automation equipment《综合建筑自动化设备用图形符号》.pdf CEN TS 15810-2008 Graphical symbols for use on integrated building automation equipment《综合建筑自动化设备用图形符号》.pdf
  • CEN TS 15844-1-2010 Postal services - ID-tagging of letter mail items - Part 1 ID-tag structure message and binary《邮政服务 ID-tagging信邮件 第1部分 ID-tag结构 消息和二进制》.pdf CEN TS 15844-1-2010 Postal services - ID-tagging of letter mail items - Part 1 ID-tag structure message and binary《邮政服务 ID-tagging信邮件 第1部分 ID-tag结构 消息和二进制》.pdf
  • CEN TS 15844-2-2010 Postal services - ID-tagging of letter mail items - Part 2 BNB-78 Encoding Specification《邮政服务 ID-tagging信邮件 第2部分 bnb - 78编码邮件规范》.pdf CEN TS 15844-2-2010 Postal services - ID-tagging of letter mail items - Part 2 BNB-78 Encoding Specification《邮政服务 ID-tagging信邮件 第2部分 bnb - 78编码邮件规范》.pdf
  • CEN TS 15844-3-2010 Postal services - ID-tagging of letter mail items - Part 3 BNB-62 encoding specification《邮政服务 ID-tagging信邮件 第3部分 bnb - 62编码规范》.pdf CEN TS 15844-3-2010 Postal services - ID-tagging of letter mail items - Part 3 BNB-62 encoding specification《邮政服务 ID-tagging信邮件 第3部分 bnb - 62编码规范》.pdf
  • 相关搜索

    当前位置:首页 > 标准规范 > 国际标准 > 其他

    copyright@ 2008-2019 麦多课文库(www.mydoc123.com)网站版权所有
    备案/许可证编号:苏ICP备17064731号-1